HG/T 2275.4-1992 Determination of moisture content of realgar ore
time:
2024-08-13 09:14:19
- HG/T 2275.4-1992
- in force
Standard ID:
HG/T 2275.4-1992
Standard Name:
Determination of moisture content of realgar ore
Chinese Name:
雄黄矿 雌黄矿水分的测定
Standard category:
Chemical industry standards (HG)
-
Date of Implementation:
1992-07-01
China Standard Classification Number:
Chemicals>>Coatings, Pigments, Dyes>>G51 Coating
alternative situation:
Replaced by GB 17513-98
Skip to download
Summary:
HG/T 2275.4-1992 Determination of moisture content of realgar ore HG/T2275.4-1992 Standard download decompression password: www.bzxz.net
Some standard content:
Chemical Industry Standard of the People's Republic of China
Determination of Realgar Ore and Orpiment
Subject Content and Scope of Application
This standard specifies the determination of moisture in realgar and orpiment products by the loss-in-weight method. This standard applies to the determination of moisture in realgar and orpiment products. 2 Method Summary
The sample is dried at 80±2℃ to constant weight, and its water content is calculated by weight loss. 3 Instruments and Apparatus
3.1 Weighing bottle: flat, with ground mouth, diameter of about 70mm, height of about 30mm. 3.2 Oven: with automatic temperature controller.
3.3 Dryer: filled with appropriate desiccant, such as color-changing silica gel, and other general laboratory instruments
4 Sample
The sample passes through a 2mm standard sieve
5 Analysis steps
HG/T2275.4—92
Weigh 50g of sample, accurate to 0.001g, and place it in a weighing bottle that has been dried to constant weight at 80±2℃ in advance. Shake the weighing bottle gently to spread the sample evenly in the weighing bottle, open the bottle cap, and put it in an oven at 80±2℃ to dry for 2h. Take out the weighing bottle, cover it with the cap, and put it in a dryer to cool to room temperature and weigh it. Repeat the operation (drying time is 0.5h) until the difference between the two weighings is no more than 0.002g.
Weigh two samples each time for parallel determination. 6. Expression of analysis results
The moisture content X expressed as mass percentage is calculated according to formula (1): m
Where: m—mass of sample plus weighing bottle before drying, g;—mass of sample plus weighing bottle after drying, g; m2
mass of sample, g.
The arithmetic result of parallel determination is taken The average value is taken as the determination result. The allowable difference of the parallel determination results is shown in the following table. Approved by the Ministry of Chemical Industry of the People's Republic of China on March 12, 19928
Standard access network ww.bono.cm(1)
Implementation on July 1, 1992
Additional instructions:bzxz.net
Moisture (H,0)
HG/T2275.4—92
This standard is proposed by the Science and Technology Department of the Ministry of Chemical Industry of the People's Republic of China. This standard is under the jurisdiction of the Chemical Industry and Mining Design Institute of the Ministry of Chemical Industry. This standard is drafted by the Chemical Industry and Mining Design Institute of the Ministry of Chemical Industry. The main drafters of this standard are Wang Hailiang, Min Yuyao and Zhao Zhiquan. The standard investment network.oww.bzeopo.com Various standard industry materials are free to download and fill the allowable difference
Tip: This standard content only shows part of the intercepted content of the complete standard. If you need the complete standard, please go to the top to download the complete standard document for free.
Determination of Realgar Ore and Orpiment
Subject Content and Scope of Application
This standard specifies the determination of moisture in realgar and orpiment products by the loss-in-weight method. This standard applies to the determination of moisture in realgar and orpiment products. 2 Method Summary
The sample is dried at 80±2℃ to constant weight, and its water content is calculated by weight loss. 3 Instruments and Apparatus
3.1 Weighing bottle: flat, with ground mouth, diameter of about 70mm, height of about 30mm. 3.2 Oven: with automatic temperature controller.
3.3 Dryer: filled with appropriate desiccant, such as color-changing silica gel, and other general laboratory instruments
4 Sample
The sample passes through a 2mm standard sieve
5 Analysis steps
HG/T2275.4—92
Weigh 50g of sample, accurate to 0.001g, and place it in a weighing bottle that has been dried to constant weight at 80±2℃ in advance. Shake the weighing bottle gently to spread the sample evenly in the weighing bottle, open the bottle cap, and put it in an oven at 80±2℃ to dry for 2h. Take out the weighing bottle, cover it with the cap, and put it in a dryer to cool to room temperature and weigh it. Repeat the operation (drying time is 0.5h) until the difference between the two weighings is no more than 0.002g.
Weigh two samples each time for parallel determination. 6. Expression of analysis results
The moisture content X expressed as mass percentage is calculated according to formula (1): m
Where: m—mass of sample plus weighing bottle before drying, g;—mass of sample plus weighing bottle after drying, g; m2
mass of sample, g.
The arithmetic result of parallel determination is taken The average value is taken as the determination result. The allowable difference of the parallel determination results is shown in the following table. Approved by the Ministry of Chemical Industry of the People's Republic of China on March 12, 19928
Standard access network ww.bono.cm(1)
Implementation on July 1, 1992
Additional instructions:bzxz.net
Moisture (H,0)
HG/T2275.4—92
This standard is proposed by the Science and Technology Department of the Ministry of Chemical Industry of the People's Republic of China. This standard is under the jurisdiction of the Chemical Industry and Mining Design Institute of the Ministry of Chemical Industry. This standard is drafted by the Chemical Industry and Mining Design Institute of the Ministry of Chemical Industry. The main drafters of this standard are Wang Hailiang, Min Yuyao and Zhao Zhiquan. The standard investment network.oww.bzeopo.com Various standard industry materials are free to download and fill the allowable difference
Tip: This standard content only shows part of the intercepted content of the complete standard. If you need the complete standard, please go to the top to download the complete standard document for free.
- Recommended standards
- JB/T 6276-1992 Test methods for sugar beet harvesting machinery
- GB/T 23156-2010 Packaging—Packaging and the environment—Terminology
- JT/T 1286-2020 Manufacturing practice for transferred unitized cargo of air-ground intermodal transport
- HG/T 3585-1999 Liquid sodium borohydride
- GB 15976-1995 Standard for the control and elimination of schistosomiasis in my country
- GB/T 13400.2-1992 General rule for representation on network planning techniques
- QB/T 1582-1992 Terminology of leather hardware industry
- QB 1788-1993 Hediocarbaldehyde
- HG 2271.1-1992 S201 platinum catalyst for nitric acid production
- GB/T 14837-1993 Rubber and rubber products - Determination of component content - Thermogravimetric analysis
- GB/T 15131.1-1994 130 mm floppy disks with a bit density of 13262 flux reversals/radian and 80 tracks per side for information processing data exchange Part 1: Dimensions, physical properties and magnetic properties
- GB/T 2423.24-1995 Environmental testing for electric and electronic products Part 2: Test methods Test Sa: Simulated solar radiation on the ground
- HG/T 2303-1992 Industrial Acetanilide
- HG/T 2245-1991 Various colors of nitro pencil lacquers
- GB/T 15936.8-1995 Information processing text and office systems Office document architecture (ODA) and interchange formats Part 8: Geometric content architecture
Please remember: "bzxz.net" is the combination of the first letters of the Chinese pinyin of the four Chinese characters "standard download" and the international top-level domain name ".net". ©2024 Standard download websitewww.bzxz.net Mail:bzxznet@163.com